Annealing of molded ACRYPET product
So residual stress just after quick cooling still remains in a molded product that cracks may be formed in the paint process or at the contact with solvent. To prevent such crack forming, heat a molded product to the slightly lower temperature than the formable temperature to remove this residual stress.
Standard annealing condition of molded products | |||||
Condition | VH,VHS,VH4,VH5,VH6 | MD,TF8,TF9 | MF,SV | IRG,IRK,IRL | IRD,IRS |
Air bath temperature(![]() | 85-90 | 70-75 | 65-70 | 75-85 | 65-75 |
Time(hours) | 1-3 | 1-3 | 1-3 | 1-3 | 1-3 |
Typical slow cooling speed | ||
Thickness | Slow cooling speed | |
under 4mm | 45 | |
4-9mm | 20 | |
above 9mm | 10 |